The cleaning technology of titanium alloy forgings has two aspects: one is the removal of oxide scale; the other is the removal of α shell. The rust can be removed by mechanical methods, such as sandblasting; or chemical methods, such as molten salt removal. The choice of rust removal method depends on the size, complexity, and cost of the part.
Sandblasting is an effective way to remove rust. It can remove 0.13~0.76mm thick rust. 100~150 mesh zircon sand or steel grit can be used, and the air pressure can reach 275Pa. Although sandblasting can be used for forgings of various sizes, it is mostly used for medium and large titanium alloy forgings. Sandblasting equipment can use rollers with abrasives, shot blasting, or sandblasting devices. Pickling is required after sandblasting to remove the α shell layer.
Salt-dissolving descaling is another effective method to remove oxide scale, and acid washing is also followed to remove the alpha shell layer. A flow chart, solution composition, and related parameters that usually use dissolved salt to remove rust and pickling. The shelf used for rust removal with molten salt is generally made of wood, titanium, or stainless steel to prevent electric potential from being generated between the workpiece and the shelf, which may cause electrical erosion or arcing on the workpiece. Dissolving salt rust removal is often used for medium and small forgings. In the case of large batches of forgings, the operating system can be fully automated.
Pickling is used to remove the α shell layer under the rust. The process is as follows:
(1) Use sandblasting or alkali salt for overall cleaning.
(2) If alkali cleaning is used, it should be fully cleaned in clean running water.
(3) Pickling in an aqueous solution of sand acid-hydrofluoric acid for 5-15 minutes. The solution contains 15% to 40% HNO3, 1% to 5% HF, and the operating temperature is 25 to 60°C. Usually, the acid content (especially for α+β and β alloys) usually takes the middle value of the above acid content range (for example, 30%-35% HNO3, 2%-3%HF, or the ratio of HNO3 to HF is 10:1-15:1). However, the chemical solution of HNO3 and HF of about 2:1 can achieve the removal effect of 0.025mm/min and absorbs less hydrogen.
When mixed acid is used, the titanium content in the acid solution is continuously increased, which reduces the pickling effect. It is generally considered that the titanium content of 12g/L is already the upper limit, and the solution should be discarded if it exceeds this value. Solution treatment can be carried out by filtering or adding other organic chemical additives to extend the life of the pickling solution.
(4) Thoroughly clean the forgings in clean water.
(5) Wash with hot water to accelerate drying, and let it dry after washing.
The time required for metal removal and cleaning during pickling is mainly determined by several factors including the thickness of the alpha shell, the operating conditions of the pickling tank, the need for process technical conditions, and the tendency of the workpiece to absorb hydrogen. Pickling provides conditions for excessive hydrogen absorption of titanium alloys, so it must be carefully controlled. The metal removal rate in pickling is generally 0.03mm/min or more. This rate is strongly affected by the following factors, such as alloy type, acid concentration, solution temperature, and titanium content. Metal removal thickness of 0.25~0.38mm on each surface is usually enough to remove the α shell layer. However, sometimes more or less removal may be required, depending on the type of alloy and the specific conditions of the forging being processed.
In pickling, the hydrogen absorption can reach 10×10-6 for every 0.03mm of surface metal removed, which depends on the specific pickling solution and concentration temperature conditions. In the pickling, the hydrogen absorption tendency of α alloys is higher than that of (α+β) alloys. The (α+β) alloy has a smaller tendency to absorb hydrogen in pickling than the β alloy. The tendency of hydrogen absorption in pickling increases with the decrease of metal removal rate (due to the increase of titanium content in the solution); with the increase of cleaning temperature (above 60℃); and with the increase of the relative ratio of workpiece surface area to volume Increase. Generally speaking, the metal removal rate must exceed the hydrogen diffusion rate at a certain solution concentration and temperature. After cleaning, if the hydrogen content exceeds the allowable hydrogen content of 140~170cm3/100g in the forging, vacuum hydrogen removal annealing is required.
Please send an email to sales1@bjjfti.com if need, or submit your requirements at the bottom, we will reply to you within 12 hours!